Voltage Characteristics of LFP batteries

23 March 2026

Introduction

Lithium Iron Phosphate (LFP) batteries are quickly becoming a popular battery chemistry in both electric vehicles and energy storage systems, despite a lower energy density than traditional NMC chemistries. LFP has advantages in cycle life and material cost, as well as being generally more stable in comparison to NMC, making LFP relatively safer. However, thermal runaway is still a risk. Venting gases from LFP cells contain toxic compounds and can ignite if presented with an ignition source.

 

Open-Circuit Voltage

Figure 1 shows the OCV curve for an LFP cell compared to NMC and sodium-ion (Na-Ion) chemistries. Sodium Ion technology offers similar advantages in cost and safety as LFP, however is a less developed technology with lower energy density than LFP.

 

Figure 1: OCV Comparison

 

LFP operates within a much smaller voltage range compared to the other chemistries shown. This behaviour is a result of how the active material responds during a charge, explained in the section below.

 

LFP material behaviour

The flat OCV curve is due to LFP’s non-uniform chemical potential. This means LFP exists in two phases (Li-Rich and Li-Poor) in equilibrium throughout the state of charge range. At low state of charge the cathode material is predominantly composed of the Li-Rich phase. As the cell is discharged, LFP material releases lithium ions to the anode, creating the Li-Poor phase in the cathode. The ratio of Li-Rich to Li-Poor material approximately corresponds to the overall charge state of the cell.

This process is often modelled using a many-particle approach, illustrated in Figure 2, whereby the LFP material is modelled as lots of particles each moving between the phases sequentially. In order to encourage particles to change states, the potential across the cell is increased (charging) or decreased (discharging) from the equilibrium voltage to an operating equilibrium. As the particles transition between states their potential drops back to the equilibrium voltage before returning to the operating equilibrium point in it’s new phase. The vast majority of particles at any time are stable, resulting in a flat OCV curve.

 

Figure 2: Many-Particle Model equilibrium curves

 

Figures 3 and 4 show differential capacity curves taken whilst charging at C/5, plotted against cell voltage and state of charge respectively. Figure 3 highlights the energy stored is concentrated over a very small voltage range, whilst Figure 4 allows features to be more easily identified. These peaks indicate voltages at which the majority of phase transitions are occurring. The fact that there is some change during a charge or discharge indicates the operating equilibrium is changing, possibility due to increased impedances within the cell or a physical change such as an increase in temperature.

 

Figure 3: Differential Capacity vs Cell Voltage

 

Figure 4: Differential Capacity vs. State of Charge

 

Hysteresis and Voltage Behaviour

The phase state of the LFP material is also responsible for the hysteresis and memory effects seen with LFP chemistries. The hysteresis between charge and discharge can be seen in Figure 5. The magnitude of hysteresis is substantial considering the small changes in voltage through the charge range. These effects, coupled with the flat OCV curve mean state of charge determination is notoriously difficult for LFP chemistries.

 

Figure 5: Hysteresis

 

Extensive research continues to be conducted into producing accurate state of charge estimation for LFP batteries, often involving kalman filters coupled with coulomb counting and voltage modelling. However, as models get more complex they become increasingly difficult to apply in real-world on-board BMS systems, especially for lower-cost applications where LFP’s cost advantages become attractive.

Typically, lumped-parameter equivalent circuit models (ECMs) have been used to model lithium cell behaviour without the complexity of P2D or particle modelling. However, LFP voltage behaviour dictates that ECMs are required to be more complex compared to modelling NMC chemistries.

 

Figure 6: Overshoot behaviour

 

Overshoot behaviour, such as seen in Figure 6. cannot be modelled in a typical 2-RC ECM. Additionally, voltage relaxation behaviours have been observed to vary dependant on the recent history of the cell. Figures 7 and 8 show voltage change upon removing the current demand at given SoC’s during a charge and discharge respectively. It is seen that the relaxation characteristics for a given charge state are dependent on the initial charge state and direction of current flow. The results are summarised in Figure 9, showing the magnitude of relaxation voltage against charge state for both charge and discharge.

 

Figure 7: Voltage Relaxation during charge

 

Figure 8: Voltage Relaxation during discharge

 

Figure 9: Voltage Relaxation summary

 

In addition to complexities detailed above, aging characteristics and cell manufacturing variations need to be considered. Phase-change kinetics are likely to be effected by homogentity in the LFP particles used in the electrode manufacturing process. Particle size uniformity as well as the application of carbon-coating to LFP particles could influence voltage charatersitcs of the cell.

CamMotive can provide state-of-the-art test facilites combined with in-depth understanding of battery chemistries and their applications. Our sister company, Cambustion, provides analysers and testing techniques to measure and improve material properties for battery electrodes (Battery material testing & characterisation | Cambustion).

To find out more about our testing and development capabilities, connect to an expert:

More Articles

Powertrain in the Loop

Driving Innovation in Vehicle Development   In the fast-paced world of automotive engineering, the race to innovate is relentless. As manufacturers push the boundaries of performance, efficiency, and sustainability, one technology has emerged as a quiet...

E-Motor and Inverter Testing

Testing of electric motors and traction inverter systems form an essential part of the design and validation process for hybrid, BEV and fuel cell vehicles. Using high speed data acquisition, inverter performance can be evaluated from voltage and current measurements...

Sodium-Ion Battery Technology: An Overview

Sodium-Ion batteries have recently been presented as a lower-cost solution compared to equivalent lithium based chemistries. Sodium is around 1000x more abundant in the Earth’s crust compared to Lithium, making raw material cost significantly easier and cheaper....

Basics of EIS

Electrochemical-Impedance Spectroscopy (EIS) is a method of obtaining detailed information on the performance characteristics of electro-chemical cells. During EIS, the cell is exposed to an excitation signal at a given frequency. This signal can be described in...

Impedance Testing: DCIR vs EIS

Impedance is an important battery parameter during the development, manufacture and use of an automotive battery. During production, checking impedance of individual cells is a common quality control technique. These checks may be done again with assembled module...

Differential Capacity Analysis

Differential Capacity Analysis is a method of tracking the energy required to change the voltage of a cell across a constant current charge or discharge (dQ/dV). Differentiation of the charge with respect to voltage exaggerates features in the open circuit voltage...